[{"data":1,"prerenderedAt":64},["ShallowReactive",2],{"blog-solder-graping-investigation-cn":3},{"title":4,"description":5,"date":6,"lastUpdated":6,"category":7,"image":8,"imageAlt":9,"readingTime":10,"wordCount":11,"timeRequired":12,"htmlContent":13,"faq":14,"tags":30,"slug":34,"sourceLocale":35,"availableLocales":36,"jsonld":41},"回流焊后焊膏葡萄状缺陷：如何依据焊点证据判断","通过焊点图像、印刷记录、局部热证据和受控对比调查焊膏葡萄状缺陷，在批准工艺变更前核实证据。","2026-11-13","assembly",null,"",2,365,"PT2M","\u003Cp>小焊点中保留着焊料颗粒轮廓，只能称为\u003Cstrong>值得调查的葡萄状外观焊点\u003C/strong>，不能据此下诊断。仅凭外观无法证明根因是氧化、助焊剂耗尽、峰值温度不足、焊膏缺陷或其他问题。首先确认这些颗粒是否属于焊点本身，然后将印刷证据和局部热证据与未受影响的位置进行比较，再决定是否批准受控变更。\u003C/p>\n\u003Cp>关于散落的焊球、焊珠，以及组件周围未聚合颗粒的更广泛调查，请参阅\u003Ca href=\"/cn/blog/solder-balls-smt-reflow/\">SMT 回流焊中的焊球\u003C/a>。葡萄状缺陷调查的范围更窄：\u003Cstrong>形貌和现有证据对特定焊点的聚合情况说明了什么\u003C/strong>。\u003C/p>\n\u003Ch2>首要判断：可疑特征是什么？\u003C/h2>\n\u003Cp>移动或返修电路板之前，先记录板上位置和焊点位置。负责质量的人员应依据项目要求，决定是否需要在返修或放行前进一步检查或暂扣产品。仅凭一张闪亮球体的近照不足以分类；关键是材料相对于预定焊盘、元件端头和焊点的位置。\u003C/p>\n\u003Ctable>\n\u003Cthead>\n\u003Ctr>\n\u003Cth>观察结果\u003C/th>\n\u003Cth>初步分类\u003C/th>\n\u003Cth>下一步检查\u003C/th>\n\u003C/tr>\n\u003C/thead>\n\u003Ctbody>\u003Ctr>\n\u003Ctd>小焊点的焊料中保留着颗粒轮廓\u003C/td>\n\u003Ctd>葡萄状外观焊点\u003C/td>\n\u003Ctd>将该焊点与对应的印刷情况、相邻焊点及热证据进行比较。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>电路板表面有一个与预定焊点分离的球体\u003C/td>\n\u003Ctd>散落焊球\u003C/td>\n\u003Ctd>与焊点聚合情况分开检查其位置、尺寸和分布。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>较大的球体位于元件或焊点旁\u003C/td>\n\u003Ctd>可能是焊珠\u003C/td>\n\u003Ctd>检查它是与焊点分离、附着于焊点，还是从焊点中析出。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>焊料没有按预期铺展或结合到焊盘或端头上\u003C/td>\n\u003Ctd>可能未润湿\u003C/td>\n\u003Ctd>检查暴露表面和界面；同一焊点可能既存在润湿不良，也保留着颗粒。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>焊点似乎未充分熔合，且有证据表明其局部受热可能不足\u003C/td>\n\u003Ctd>可能受热不足\u003C/td>\n\u003Ctd>结合测量位置，将实测热证据与适用的材料要求进行比较。\u003C/td>\n\u003C/tr>\n\u003C/tbody>\u003C/table>\n\u003Cp>以上只是初步分类，不是验收结论。反光、残留物和有限的观察角度都可能遮挡焊点边界。条件允许时，应从多个有用角度拍摄带比例尺的图像。经批准的切片可能有助于显示焊点结构和界面，但无法还原完整的温度或助焊剂历程。\u003C/p>\n\u003Cp>关于界面润湿状态的区别，请参阅\u003Ca href=\"/cn/blog/solder-non-wetting-vs-dewetting/\">焊料未润湿与退润湿\u003C/a>。\u003C/p>\n\u003Cp>单张图像不能证明焊点质量。仅凭电气导通也不能证明焊点质量：即使存在导电通路，焊点的机械或冶金状态仍可能需要评估。\u003C/p>\n\u003Ch2>建立与位置对应的证据记录\u003C/h2>\n\u003Cp>从受影响的焊点开始，然后选择确实具有可比性的未受影响位置：最好是同一电路板上以及其他电路板上采用相同元件和焊点设计的位置（如有）。也要纳入附近存在差异的焊点，因为这种对比可能比收集一批缺陷照片更有参考价值。\u003C/p>\n\u003Cp>返修前记录以下信息：\u003C/p>\n\u003Cul>\n\u003Cli>电路板身份和版本、生产批次或批号、拼板位置，以及元件位号和焊点位置。\u003C/li>\n\u003Cli>受影响和未受影响位置的带比例尺图像，并包含足够的周边区域以显示焊点边界。\u003C/li>\n\u003Cli>焊膏的准确产品和批次，以及现有的储存、开封、准备、处理和暴露记录。\u003C/li>\n\u003Cli>钢网版本，以及尽可能与相应位置对应的实际印刷证据，而不只是预定开口设计。\u003C/li>\n\u003Cli>相关的实装热测量、仪器固定位置和条件、电路板装载情况、炉温曲线设定及运行标识。\u003C/li>\n\u003Cli>任何缺失的记录、先前处理或返修，以及可能限制比较有效性的事项。\u003C/li>\n\u003C/ul>\n\u003Cp>如果某项记录、合适的对比位置或测量不存在，应标记为\u003Cstrong>未知\u003C/strong>。不要用标称炉温曲线或假定的工艺条件代替实测证据。\u003C/p>\n\u003Ch3>印刷证据不等于回流后的结果\u003C/h3>\n\u003Cp>贴装前的对应位置图像或\u003Ca href=\"/cn/blog/solder-paste-inspection-spi/\">焊膏检测（SPI）\u003C/a>结果，有助于确认是否印有焊膏，并可根据检测能力描述焊膏沉积情况。但它无法证明最终焊点在回流后是否完成聚合。\u003C/p>\n\u003Cp>将受影响位置的实际沉积情况与匹配的未受影响位置进行比较。判断证据显示的是可重复的印刷差异，还是最终焊点中仅有感知上的差异。如果检测覆盖范围或位置映射不完整，这项比较也就不完整。\u003C/p>\n\u003Cp>钢网设计可能与问题有关，但开口图纸无法证明实际印刷结果。若没有适用的设计要求和产品要求，也不应把开口面积比当作通用的合格/不合格判定规则。\u003C/p>\n\u003Ch3>设定温度不等于焊点温度\u003C/h3>\n\u003Cp>炉温设定值描述的是已编程的环境温度，并非实测焊点温度。将热电偶正确安装在具有代表性的实装电路板上，记录的是\u003Cstrong>其实际安装位置和安装状态下\u003C/strong>的温度，并不能测量每一个隐藏焊点。\u003C/p>\n\u003Cp>如果已有实装炉温曲线，应核对电路板装载情况、热电偶安装是否牢固，以及测点与调查位置的接近程度。将曲线与焊膏、元件和 PCB 制造商适用的温度及暴露时间限值进行比较。如果没有相关炉温曲线，热学假设仍未得到验证；若有合适的电路板和设备，应安排经批准的测量。\u003C/p>\n\u003Cp>关于测量设置和安装证据，请参阅\u003Ca href=\"/cn/blog/reflow-thermocouple-attachment-profiling/\">回流焊炉温曲线测量中的热电偶安装\u003C/a>。\u003C/p>\n\u003Cp>本调查不存在通用的预热、升温速率、峰值、气氛或暴露时间设定。对某个焊点有帮助的变更，可能在其他位置引发问题，或超出材料限值。\u003C/p>\n\u003Ch2>先比较各种解释，再选择变更\u003C/h2>\n\u003Cp>需要特别区分以下两种热状态：\u003C/p>\n\u003Col>\n\u003Cli>**受热不足：**局部焊料可能未达到焊点所需的熔化条件。\u003C/li>\n\u003Cli>**已经熔化但未能聚合：**部分或全部焊料可能已经熔化，但最终焊点仍保留着彼此分离的颗粒轮廓。\u003C/li>\n\u003C/ol>\n\u003Cp>附近热电偶曲线超过焊膏合金标示的液相线，并不能单独证明第二种状态。隐藏焊点的情况可能与热电偶安装点不同，而且曲线无法直接显示各颗粒发生了什么。反过来，最终形状不美观，也不能证明焊料从未熔化。\u003C/p>\n\u003Cp>下表将外观转化为相互竞争的待验证假设，而不是一份预设根因清单。\u003C/p>\n\u003Ctable>\n\u003Cthead>\n\u003Ctr>\n\u003Cth>观察到的证据\u003C/th>\n\u003Cth>相互竞争的假设\u003C/th>\n\u003Cth>区分性检查\u003C/th>\n\u003Cth>局限\u003C/th>\n\u003C/tr>\n\u003C/thead>\n\u003Ctbody>\u003Ctr>\n\u003Ctd>小焊点保留着颗粒轮廓\u003C/td>\n\u003Ctd>局部焊料受热不足；或者已经熔化但未完全聚合\u003C/td>\n\u003Ctd>根据焊膏合金资料和适用的产品限值，审查相关实测炉温曲线。若可行且获得批准，可在具有代表性的设置中进行直接过程观察。\u003C/td>\n\u003Ctd>热电偶报告的是其安装点温度；观察可能无法看到生产中的隐藏焊点。两者都不能自动证明每个颗粒的热历程。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>某些焊点呈葡萄状外观，而匹配焊点没有\u003C/td>\n\u003Ctd>特定位置的印刷差异有所影响；或者贴装或局部加热存在差异\u003C/td>\n\u003Ctd>比较受影响和未受影响位置对应的贴装前沉积图、元件位置及局部周边情况。\u003C/td>\n\u003Ctd>缺失或不匹配的图像会使比较无法得出结论；外观正常的印刷结果也不能证明焊料已聚合。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>多个受影响焊点集中在某块电路板或某个拼板位置\u003C/td>\n\u003Ctd>电路板位置或局部热条件有所影响；或者发生了共同的印刷或处理事件\u003C/td>\n\u003Ctd>按电路板、拼板位置和运行批次映射焊点结果，并与相关实测炉温曲线和印刷记录比较。\u003C/td>\n\u003Ctd>同一块电路板上的焊点不能作为证明板级根因的相互独立证据。少量聚集现象可能有多种解释。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>可疑焊点出现在焊膏处理间隔之后\u003C/td>\n\u003Ctd>焊膏状态或助焊剂行为可能有所影响；或者该时间段恰逢其他工艺变化\u003C/td>\n\u003Ctd>审查产品和批次处理记录；如获批准，可在匹配位置上对不同焊膏状态进行受控比较。\u003C/td>\n\u003Ctd>外观不能证明发生了氧化、助焊剂耗尽或焊膏不良。对比结果仍可能受到时间或设置变化的干扰。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>焊料未覆盖焊盘或端头的一部分\u003C/td>\n\u003Ctd>可能存在未润湿；或者焊料供给量有限或贴装情况影响了表观覆盖\u003C/td>\n\u003Ctd>比较印刷和贴装证据；适当时检查界面或经批准的切片。\u003C/td>\n\u003Ctd>仅凭表面外观可能无法识别机理，也无法判定是否合格。\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>附近炉温曲线显示已达到熔化条件，但焊点仍呈颗粒状\u003C/td>\n\u003Ctd>局部已熔化但未完全聚合的解释具有可能性；局部受热不足仍不能排除\u003C/td>\n\u003Ctd>复核热电偶的安装位置和状态，然后在实际可行时寻找更接近的代表性测量或直接观察。\u003C/td>\n\u003Ctd>附近的曲线不能证明隐藏焊点的温度，也不能证实单一根因。\u003C/td>\n\u003C/tr>\n\u003C/tbody>\u003C/table>\n\u003Cp>颗粒尺寸和气氛可能与特定的已批准工艺相关，但不能仅凭外观变更这两项，也不能为它们指定通用设定。下一步应选择最有可能区分主要解释、同时又能保留现有证据的检查。\u003C/p>\n\u003Cp>Indium Corporation 的《Minimizing Graping》讨论了沉积形状、氧化、助焊剂和热暴露等相互作用因素。AIM Solder 的《W20 SAC305》案例研究同时描述了焊膏和炉温曲线的变更，因此无法单独分辨其中任何一个因素，也不能为其他组件提供验证。试验前应核对实际使用的焊膏、元件和 PCB 文档及项目要求。\u003C/p>\n\u003Ch2>虚构对比示例：对相同位置计数\u003C/h2>\n\u003Cp>以下示例为虚构内容，旨在展示如何组织对比。它不是客户结果、真实测试，也不代表良率提升或因果关系。\u003C/p>\n\u003Cp>调查人员将统计单位定义为\u003Cstrong>一个具名焊点位置\u003C/strong>。基线组使用拼板位置为 A、B、C 的三块电路板；试验组使用拼板位置相同、与之匹配的三块电路板。每块板评估 4 个对应焊点位置，因此每组共计 12 个位置。每个位置按外观分类为 \u003Cstrong>G\u003C/strong>（葡萄状外观）或 \u003Cstrong>C\u003C/strong>（未观察到葡萄状外观）。该分类不代表质量处置结论。\u003C/p>\n\u003Ctable>\n\u003Cthead>\n\u003Ctr>\n\u003Cth>匹配的电路板位置\u003C/th>\n\u003Cth>基线组：位置 1–4\u003C/th>\n\u003Cth align=\"right\">基线组 G 数量\u003C/th>\n\u003Cth>试验组：位置 1–4\u003C/th>\n\u003Cth align=\"right\">试验组 G 数量\u003C/th>\n\u003C/tr>\n\u003C/thead>\n\u003Ctbody>\u003Ctr>\n\u003Ctd>A\u003C/td>\n\u003Ctd>G, G, C, C\u003C/td>\n\u003Ctd align=\"right\">4 个中有 2 个\u003C/td>\n\u003Ctd>G, C, C, C\u003C/td>\n\u003Ctd align=\"right\">4 个中有 1 个\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>B\u003C/td>\n\u003Ctd>G, C, C, C\u003C/td>\n\u003Ctd align=\"right\">4 个中有 1 个\u003C/td>\n\u003Ctd>G, C, C, C\u003C/td>\n\u003Ctd align=\"right\">4 个中有 1 个\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>C\u003C/td>\n\u003Ctd>G, G, C, C\u003C/td>\n\u003Ctd align=\"right\">4 个中有 2 个\u003C/td>\n\u003Ctd>G, C, C, C\u003C/td>\n\u003Ctd align=\"right\">4 个中有 1 个\u003C/td>\n\u003C/tr>\n\u003Ctr>\n\u003Ctd>\u003Cstrong>合计\u003C/strong>\u003C/td>\n\u003Ctd>\u003C/td>\n\u003Ctd align=\"right\">\u003Cstrong>12 个中有 5 个\u003C/strong>\u003C/td>\n\u003Ctd>\u003C/td>\n\u003Ctd align=\"right\">\u003Cstrong>12 个中有 3 个\u003C/strong>\u003C/td>\n\u003C/tr>\n\u003C/tbody>\u003C/table>\n\u003Cp>虚构记录显示，两组使用相同的电路板版本、钢网版本、焊膏产品和批次，并记录了两组的处理情况。贴装前的对应位置图像显示，所有 24 个评估位置均有焊膏，但没有沉积体积测量数据。这只能支持焊膏是否存在的比较，不能得出印刷效果相同的结论。\u003C/p>\n\u003Cp>针对试验，产品工程部门批准\u003Cstrong>变更一个炉区的设定值\u003C/strong>以作调查；其他炉温曲线设定按记录保持不变。每种条件都运行一块已装配元件的测量板。两次运行中，记录的安装点曲线均超过焊膏合金标示的液相线；试验曲线与基线曲线有所不同。试验前已审查适用的焊膏、元件和 PCB 限值。这些曲线无法确定 24 个受评焊点各自的温度。\u003C/p>\n\u003Cp>团队还检查了每组 12 个匹配的相邻焊点是否存在可见桥连：基线组和试验组均为 \u003Cstrong>12 个中有 0 个\u003C/strong>。这是范围有限的目视观察，不能证明不存在其他缺陷或可靠性方面的权衡。\u003C/p>\n\u003Cp>试验组的葡萄状外观减少了两个：5 减 3 等于 2。但每组只比较了三块板，且每块板上包含多个位置。板级相关性、运行顺序、未测量的印刷差异和隐藏焊点温度都仍可能造成影响。在这个虚构样本中，变更与数量减少相关；这\u003Cstrong>不能\u003C/strong>证明唯一根因，也不能作为放行决定的依据。\u003C/p>\n\u003Ch2>验证受控变更\u003C/h2>\n\u003Cp>选定一个主要假设，并事先说明哪些观察结果会支持该假设、哪些会削弱它，以及哪些信息仍无法测量。例如，如果主要关注局部热暴露，应在调整炉温曲线前定义比较位置和热电偶安装方式。如果主要关注印刷差异，应在更改钢网或印刷机设置前保留对应的印刷证据。\u003C/p>\n\u003Cp>使用匹配的基线，并在可行时一次只做\u003Cstrong>一项获批变更\u003C/strong>。记录无法保持一致的其他差异，包括焊膏暴露时间、电路板装载情况、拼板位置和运行顺序。单独改变一个设定值仍可能改变热曲线的多个方面；因此应记录所得炉温曲线，而不能只用变更的设定值来描述试验。\u003C/p>\n\u003Cp>在基线和试验中评估相同的具名位置，并采用相同的观察方法。同时监测相关的相邻缺陷和潜在权衡，例如可见桥连、其他焊点的变化或可能的热暴露问题。不能以牺牲电路板上未经检查的区域为代价，换取某个小焊点的改善。\u003C/p>\n\u003Cp>适当且可行时，应重复或扩大比较，并考虑到各焊点共用电路板、拼板和工艺运行。若证据互相矛盾或缺少关键测量，应保留不确定性。变更后出现改善是有用证据，但单凭相关性不能证明变更因素是唯一原因。\u003C/p>\n\u003Ch2>区分调查、工程和质量决策\u003C/h2>\n\u003Cul>\n\u003Cli>**调查人员：**保全并整理证据、对观察结果分类、比较假设、报告缺失信息，并提出有区分力的检查。\u003C/li>\n\u003Cli>**产品工程：**判断哪些测量或试验变更在技术上适当，并在适用的材料和产品限制范围内批准实施。\u003C/li>\n\u003Cli>**质量部门：**依据适用的客户要求评估所得证据并处置产品。记录任何放行决定及其依据。\u003C/li>\n\u003C/ul>\n\u003Cp>不要把目视分类、导通读数或试验改善视为自动放行依据。\u003C/p>\n\u003Ch2>询价或调查交接\u003C/h2>\n\u003Cp>如需讨论\u003Ca href=\"/cn/products/pcb-assembly/\">PCB 组装\u003C/a>或\u003Ca href=\"/cn/quote/\">获取报价\u003C/a>，请提供现有资料，并注明缺失项：\u003C/p>\n\u003Col>\n\u003Cli>电路板身份和版本、生产标识、拼板位置、元件位号及准确焊点位置。\u003C/li>\n\u003Cli>返修前受影响和未受影响焊点的带比例尺图像，并标出预定焊点边界。\u003C/li>\n\u003Cli>焊膏的准确产品、批次以及现有储存和处理记录。\u003C/li>\n\u003Cli>钢网版本、印刷设置记录，以及对应的实际印刷或 SPI 证据，包括检测覆盖范围。\u003C/li>\n\u003Cli>实装炉温曲线文件或测量数据、电路板装载情况、热电偶安装位置和条件，以及炉温曲线设定和运行标识。\u003C/li>\n\u003Cli>适用的焊膏、元件和 PCB 要求，以及客户的验收和处置要求。\u003C/li>\n\u003Cli>任何拟议的受控对比、相关相邻缺陷、先前返修情况和已知证据缺口。\u003C/li>\n\u003C/ol>\n\u003Cdiv data-component=\"BlogQuickQuoteInline\">\u003C/div>\n\n\u003C!-- faq:start -->\n\n\u003Ch2>常见问题\u003C/h2>\n\u003Ch3>所有看起来有颗粒感的焊点都是焊膏葡萄状缺陷吗？\u003C/h3>\n\u003Cp>不是。保留着颗粒轮廓，可以合理描述为葡萄状聚合外观，但残留物、反光或不完整的视野都可能造成误判。应确认材料相对于焊盘和端头的位置，并区分焊点材料与散落的焊球或焊珠。\u003C/p>\n\u003Ch3>葡萄状缺陷能证明回流焊峰值温度太低吗？\u003C/h3>\n\u003Cp>不能。受热不足只是其中一种可能。焊料也可能已经熔化，却仍未充分聚合。应使用相关的实测热证据，并注意热电偶无法报告每一个隐藏焊点的温度。\u003C/p>\n\u003Ch3>SPI 能确认回流后的焊点良好吗？\u003C/h3>\n\u003Cp>不能。SPI 根据其检测覆盖范围描述贴装前的印刷情况。它可以支持对焊膏沉积的比较，但回流后的检查以及任何其他规定的评估都需要分别进行。\u003C/p>\n\u003Ch3>是否应该立即更改炉温曲线？\u003C/h3>\n\u003Cp>不能仅因焊点看起来有颗粒感就更改。先保留证据，审查适用的材料限值，并比较主要假设。随后，产品工程人员可批准在匹配基线和权衡监测下进行受控变更。\u003C/p>\n\u003Ch3>如果没有炉温曲线或可用的印刷记录怎么办？\u003C/h3>\n\u003Cp>记录这些缺口，并将相关假设保留为未决。如果具备合适资源，应安排经批准的测量或对比，而不是把炉温设定值或钢网设计当作实际情况的证明。\u003C/p>\n\u003C!-- faq:end -->\n\u003Csection class=\"related-links\" aria-label=\"相关链接\">\u003Ch3 id=\"related-links\">相关链接\u003C/h3>\u003Cul>\u003Cli>\u003Ca href=\"/cn/blog/solder-balls-smt-reflow/\">SMT 回流焊中的锡珠：成因与预防\u003C/a>\u003C/li>\u003Cli>\u003Ca href=\"/cn/blog/solder-non-wetting-vs-dewetting/\">焊料不润湿与退润湿：如何诊断两种现象\u003C/a>\u003C/li>\u003Cli>\u003Ca href=\"/cn/blog/solder-paste-inspection-spi/\">什么是锡膏检测（SPI）？测量指标、判定准则与印刷放行机制\u003C/a>\u003C/li>\u003Cli>\u003Ca href=\"/cn/blog/reflow-thermocouple-attachment-profiling/\">PCB 回流焊温度曲线中的热电偶固定方法\u003C/a>\u003C/li>\u003Cli>\u003Ca href=\"/cn/products/pcb-assembly/\">PCB 组装\u003C/a>\u003C/li>\u003Cli>\u003Ca href=\"/cn/quote/\">获取报价\u003C/a>\u003C/li>\u003C/ul>\u003C/section>",[15,18,21,24,27],{"question":16,"answer":17,"answerText":17},"所有看起来有颗粒感的焊点都是焊膏葡萄状缺陷吗？","不是。保留着颗粒轮廓，可以合理描述为葡萄状聚合外观，但残留物、反光或不完整的视野都可能造成误判。应确认材料相对于焊盘和端头的位置，并区分焊点材料与散落的焊球或焊珠。",{"question":19,"answer":20,"answerText":20},"葡萄状缺陷能证明回流焊峰值温度太低吗？","不能。受热不足只是其中一种可能。焊料也可能已经熔化，却仍未充分聚合。应使用相关的实测热证据，并注意热电偶无法报告每一个隐藏焊点的温度。",{"question":22,"answer":23,"answerText":23},"SPI 能确认回流后的焊点良好吗？","不能。SPI 根据其检测覆盖范围描述贴装前的印刷情况。它可以支持对焊膏沉积的比较，但回流后的检查以及任何其他规定的评估都需要分别进行。",{"question":25,"answer":26,"answerText":26},"是否应该立即更改炉温曲线？","不能仅因焊点看起来有颗粒感就更改。先保留证据，审查适用的材料限值，并比较主要假设。随后，产品工程人员可批准在匹配基线和权衡监测下进行受控变更。",{"question":28,"answer":29,"answerText":29},"如果没有炉温曲线或可用的印刷记录怎么办？","记录这些缺口，并将相关假设保留为未决。如果具备合适资源，应安排经批准的测量或对比，而不是把炉温设定值或钢网设计当作实际情况的证明。",[31,32,33],"SMT 组装","焊膏","回流焊缺陷","solder-graping-investigation","cn",[37,38,35,39,40],"en","de","fr","ru",{"blog":42,"breadcrumb":51},{"@context":43,"@type":44,"headline":4,"description":5,"url":45,"datePublished":6,"dateModified":6,"timeRequired":12,"keywords":46,"articleSection":7,"author":47,"publisher":50},"https://schema.org","BlogPosting","https://hilpcb.com/cn/blog/solder-graping-investigation/","SMT 组装, 焊膏, 回流焊缺陷",{"@type":48,"name":49},"Organization","HILPCB",{"@type":48,"name":49},{"@context":43,"@type":52,"itemListElement":53},"BreadcrumbList",[54,59,62],{"@type":55,"position":56,"name":57,"item":58},"ListItem",1,"Home","https://hilpcb.com/",{"@type":55,"position":10,"name":60,"item":61},"Blog","https://hilpcb.com/cn/blog/",{"@type":55,"position":63,"name":34,"item":45},3,1795146117726]